ENG 204 · Basic Engineering Materials
Our notes
2 min readPhases
| Phase | Structure | Max carbon | Notes |
|---|---|---|---|
| Ferrite (α) | BCC | 0.022 wt% at 727 °C | soft, ductile, magnetic |
| Austenite (γ) | FCC | 2.14 wt% at 1,147 °C | soft, non-magnetic; stable only at high temperature in plain steels |
| Cementite (Fe₃C) | compound | 6.70 wt% | very hard, brittle |
| δ-ferrite | BCC | small | above 1,394 °C |
Steels contain up to about 2.14 wt% C; cast irons 2.14 to 6.70 (usually 3 to 4.5).
Key reactions
- Eutectoid (727 °C, 0.76 wt% C): γ → α + Fe₃C. The product is pearlite: fine alternating plates of ferrite and cementite; strong and reasonably tough.
- Eutectic (1,147 °C, 4.30 wt% C): L → γ + Fe₃C (ledeburite): basis of cast irons.
Classes of steel by carbon
- Hypoeutectoid (< 0.76% C): proeutectoid ferrite + pearlite. Mild steel (about 0.15-0.25% C) for structures and bolts.
- Eutectoid (0.76% C): all pearlite.
- Hypereutectoid (0.76-2.14% C): proeutectoid cementite (at grain boundaries) + pearlite. Tool steels.
More carbon means more cementite: harder and stronger, less ductile and weldable.
Lever rule examples
Worked example 1: 0.40 wt% C steel just below 727 °C
Proeutectoid ferrite: W_α′ = (0.76 − 0.40)/(0.76 − 0.022) = 0.36/0.738 = 0.49.
Pearlite: W_p = (0.40 − 0.022)/0.738 = 0.51.
Total ferrite (including that in pearlite): W_α = (6.70 − 0.40)/(6.70 − 0.022) = 0.94; cementite 0.06.
Worked example 2: eutectoid steel
Ferrite in pearlite = (6.70 − 0.76)/(6.70 − 0.022) = 0.89; cementite 0.11: pearlite is mostly ferrite with thin cementite plates.
Cast irons
- White iron: carbon as cementite; hard, brittle, wear-resistant.
- Grey iron: carbon as graphite flakes; machinable, damps vibration, weak in tension (engine blocks, machine beds).
- Ductile (nodular) iron: graphite spheres (magnesium added); strong and ductile (pipes, crankshafts).
- Malleable iron: white iron heat-treated to graphite clusters.
Effects of alloying elements
Mn, Ni, Cr, Mo shift the eutectoid temperature and composition and slow transformations (improving hardenability). Stainless steels need at least about 10.5% Cr.
Exams usually ask
- Sketch the Fe-Fe₃C diagram, labelling phases, temperatures and compositions.
- Describe the cooling of hypo-, hyper- and eutectoid steels and their microstructures.
- Calculate phase fractions with the lever rule.
Common mistake
Using 0.8% or 0.83% C and 723 °C from old books without saying so. Modern data give 0.76 wt% C and 727 °C; follow the values your lecturer uses but be consistent.
Written by the UniHive team in our own words. Spotted a mistake? Tell us on WhatsApp.
Read
-
Steel
(opens en.wikipedia.org in a new tab)
Wikipedia, Steel, CC BY-SA 4.0 · licence
-
Cementite
(opens en.wikipedia.org in a new tab)
Wikipedia, Cementite, CC BY-SA 4.0 · licence
-
Austenite
(opens en.wikipedia.org in a new tab)
Wikipedia, Austenite, CC BY-SA 4.0 · licence
Watch
-
Best pick Iron Carbon Phase Diagram
8 min · ≈ 36 MB · about ₦20
(opens youtube.com in a new tab)
-
Iron-Carbon Phase Diagram simply explained Part I | Creating | Steel | Cast Iron
16 min · ≈ 72 MB · about ₦40
(opens youtube.com in a new tab)
-
Lecture 19: Iron-carbon phase diagram
28 min · ≈ 126 MB · about ₦71
(opens youtube.com in a new tab)
-
The Iron Carbon Phase Diagram || Part 1
17 min · ≈ 77 MB · about ₦43
(opens youtube.com in a new tab)
-
#62 Phase Diagrams | Iron Iron Carbide Phase Diagram | Basics of Materials Engineering
41 min · ≈ 185 MB · about ₦104
(opens youtube.com in a new tab)
We link to free material and never copy it. Every link was opened by our team before it went up; video data is a rough guide at 360p.