UNIHIVE

Study Hub UNIPORT CHE 315

CHE 315 · Transport Phenomena I

Diffusion in solids

Steady diffusion through membranes and walls, Fick's second law, case hardening of steel by the error-function solution, and porous solids.

Our notes

2 min read

Mechanisms

  • Interstitial diffusion: small atoms (H, C, N) jump between gaps in a metal lattice; fairly fast.
  • Vacancy diffusion: atoms jump into empty lattice sites; slower.
  • Diffusion in polymers: gases and liquids dissolve and move between chains (packaging films, membranes).
  • Porous solids (catalysts, adsorbents, soils): diffusion through the pores, in the gas or liquid filling them.

Diffusivity in solids rises strongly with temperature: D = D₀ e^{−Q/RT} (Arrhenius).

Steady diffusion through a wall or membrane

N_A = D (C₁ − C₂) / L
where C₁, C₂ are concentrations inside the solid at each face. For gases, these depend on solubility: C = S p, so N_A = D S (p₁ − p₂)/L. The product P_M = D S is the permeability.

Worked example 1: a membrane

D = 1.0 × 10⁻¹⁰ m²/s; concentrations in the solid 50 and 0 mol/m³ at the faces; thickness 1 mm.

  • N_A = 1.0 × 10⁻¹⁰ × 50 / 0.001 = 5.0 × 10⁻⁶ mol/m² s.

Halving the thickness doubles the flux.

Fick's second law

Unsteady diffusion: ∂C/∂t = D ∂²C/∂x², identical in form to unsteady conduction.

Case hardening (carburising) of steel

Steel parts (gears, shafts) are heated in a carbon-rich atmosphere so carbon diffuses into the surface, giving a hard skin and a tough core. With surface concentration C_s held constant and initial C₀:
(C_x − C₀)/(C_s − C₀) = 1 − erf(x / (2√(Dt)))

Worked example 2: how long to carburise?

Steel with 0.2 wt% carbon; surface held at 1.2 wt%; target 0.8 wt% at 0.5 mm depth; D = 1.6 × 10⁻¹¹ m²/s at the treatment temperature.

  • (0.8 − 0.2)/(1.2 − 0.2) = 0.6 = 1 − erf(z), so erf(z) = 0.4 and z = 0.371.
  • x/(2√(Dt)) = 0.371, so √(Dt) = 0.0005/(2 × 0.371) = 6.74 × 10⁻⁴ m.
  • Dt = 4.55 × 10⁻⁷ m², t = 4.55 × 10⁻⁷ / 1.6 × 10⁻¹¹ = 28,400 s (about 7.9 hours).
  • To double the depth at the same temperature takes four times as long (t ∝ x²); raising the temperature raises D and shortens the time.

Porous solids

Effective diffusivity D_eff = D ε / τ, where ε is the porosity and τ the tortuosity (pores wander). In very small pores (or at low pressure) molecules hit the walls more than each other: Knudsen diffusion, D_K = (d_pore/3) √(8RT/(πM)).

Uses

Doping silicon chips, hydrogen embrittlement of steel pipelines, drying of solids (moisture diffuses to the surface), food packaging, controlled release, corrosion and oxidation of metals, and transdermal patches.

Exams usually ask

  • Steady diffusion through a solid wall or membrane; define permeability.
  • Use the error-function solution for carburising or doping problems.
  • Explain diffusion mechanisms and Knudsen diffusion.

Common mistake

Using gas-phase partial pressures directly in Fick's law for a solid. Convert to concentrations in the solid with the solubility (C = S p) first.

Written by the UniHive team in our own words. Spotted a mistake? Tell us on WhatsApp.

Read

Watch

We link to free material and never copy it. Every link was opened by our team before it went up; video data is a rough guide at 360p.

All CHE 315 topics

Report

Sign in to report this. It is free.

Is this your work (a lecturer, author or publisher)? Ask us to take it down.